Magnetic Materials, Permeability and Hysteresis
Wind 20 turns on an air former and you get about a microhenry; wind the same 20 turns on a ferrite toroid and you get a millihenry. Put a steel core in a transformer and it gets warm even with nothing connected. Lift a few grams of neodymium and it holds a kilogram of steel. All three are the material's own atomic currents adding to, or fighting, the field of the coil. This lesson models them with the magnetisation , defines permeability properly, and explains hysteresis, the loop that makes permanent magnets possible and costs energy in every AC core. The school picture of magnets is in Magnetic Field and the circuit view of cores in Magnetism and Induction.
Magnetisation, H and B
Each atom carries a tiny magnetic moment from electron spin and orbital motion. In a field these moments partly line up, and the material acquires a magnetisation , the magnetic moment per unit volume (A/m). An aligned block of moments acts like a current flowing around its surface (a bound current ), which adds to the field. The general relation is
and Ampère's law for (Ampère's Circuital Law: H and B) counts only the free currents in your wires. In a linear material with the susceptibility , so
Three kinds of response
| Class | Mechanism | Examples | |
|---|---|---|---|
| diamagnetic | about | induced orbital currents oppose the field | copper, water, bismuth, superconductors () |
| paramagnetic | to | weak alignment of atomic moments, fought by thermal motion | aluminium, oxygen, platinum |
| ferromagnetic / ferrimagnetic | to , field dependent | moments aligned in domains; the field moves domain walls and rotates domains | iron, nickel, cobalt, steels, ferrites |
For dia- and paramagnets for every engineering purpose. Ferromagnets are where the action is, and for them is not a constant: it depends on , on the history of the material, on temperature and on frequency. Above the Curie temperature the domains vanish and the material becomes paramagnetic (iron at about ; manganese-zinc power ferrites at only about to , and high-permeability grades lower still, a real limit for hot power inductors).
The hysteresis loop
Drive a ferromagnet with a coil current that goes up and down, and does not retrace its path. Starting from a demagnetised state, climbs steeply and then saturates at when all domains are aligned (beyond that grows only as ). Reduce to zero and stays at the remanence ; it takes a reverse field, the coercivity , to bring back to zero. The closed curve is the hysteresis loop.
- Soft materials (silicon steel, ferrites, nanocrystalline and amorphous alloys) have a narrow loop: small , high permeability, low loss per cycle. They go into transformers, inductors, motors and shields.
- Hard materials (NdFeB, SmCo, hard ferrite, AlNiCo) have a wide loop: large , high . A large coercivity is exactly what lets a magnet keep its magnetisation against its own demagnetising field: permanent magnets.
Hysteresis loss. The energy the coil delivers per unit volume while changes is . Around a closed loop the stored part comes back, and the loop area is lost as heat each cycle:
So hysteresis loss rises in proportion to frequency at a fixed flux swing. Add the eddy-current loss (currents induced in the conducting core, rising with ; reduced by thin insulated laminations or by non-conducting ferrite; Faraday's and Lenz's Laws) and you get the core loss in datasheets. Designers fit it with the empirical Steinmetz equation , with typically to and typically to over a fitted range.
Typical materials (handbook ranges as of 2026; every grade's datasheet differs):
| Material | Typical | or | Used for |
|---|---|---|---|
| silicon steel (about 3 % Si) | to several (grain-oriented highest) | 50/60 Hz transformers, motors | |
| MnZn ferrite | to | to at , lower when hot | switch-mode transformers, 10 kHz to 1 MHz |
| NiZn ferrite | to | about | EMI beads, RF up to hundreds of MHz |
| iron powder, alloy powder | to (distributed gap) | about to | power inductors with DC bias |
| NdFeB magnet | recoil | to | motors, speakers, sensors |
| hard ferrite magnet | recoil | cheap motors, fridge magnets |
Worked example: hysteresis loss in a steel core
Given: a steel modelled by the loop in the figure: term , , cycled between at . Density . A core of .
Find: an estimate of the loss per cycle, per kilogram and for the core.
Solve: a loop that is nearly rectangular between and has area about :
Check: unit check, . Electrical steels are sold by their total loss at , : roughly to for non-oriented grades depending on grade and thickness (the grade name carries it: an M400-50A sheet is at most, IEC 60404-8-4), and grain-oriented steel is far lower, so the estimate is in the right range. A transformer's no-load loss is this core loss, paid all day whether or not anything is connected.
In Python: a model loop and its area
The code uses a simple two-branch model, (a fitted curve, not a physical theory such as Jiles–Atherton or Preisach), integrates the loop area, and reads the permeabilities off the curve.
import numpy as np
import matplotlib.pyplot as plt
MU0 = 4e-7 * np.pi
Bs, Hc, H0 = 1.5, 40.0, 100.0 # model parameters: saturation term (T), coercivity (A/m), knee width (A/m)
Hmax, f, dens = 500.0, 50.0, 7650.0 # peak field (A/m), frequency (Hz), steel density (kg/m^3)
H = np.linspace(-Hmax, Hmax, 4001)
B_up = Bs * np.tanh((H - Hc) / H0) + MU0 * H # rising branch
B_dn = Bs * np.tanh((H + Hc) / H0) + MU0 * H # falling branch
Br = Bs * np.tanh(Hc / H0)
print(f"remanence Br = {Br:.3f} T, coercivity Hc = {Hc:.0f} A/m, B at Hmax = {B_up[-1]:.3f} T")
trap = lambda y, x: float(np.sum((y[1:] + y[:-1]) * np.diff(x)) / 2)
w = abs(trap(H, B_dn) - trap(H, B_up)) # loop area = closed integral of H dB
print(f"loop area = {w:.1f} J/m^3 per cycle")
print(f"hysteresis loss at {f:.0f} Hz: {w*f/1e3:.2f} kW/m^3 = {w*f/dens:.2f} W/kg")
dBdH = np.gradient(B_up, H)
i = np.argmax(dBdH)
print(f"steepest slope at H = {H[i]:.1f} A/m: mu_r(diff) = {dBdH[i]/MU0:.0f}")
k = np.argmin(abs(H - 200))
print(f"amplitude permeability at 200 A/m: B/(mu0 H) = {B_up[k]/(MU0*H[k]):.0f}")
fig, ax = plt.subplots(figsize=(5, 3.6))
ax.plot(H, B_up, label="rising H")
ax.plot(H, B_dn, label="falling H")
ax.set_xlabel("H (A/m)"); ax.set_ylabel("B (T)"); ax.grid(True, alpha=0.3); ax.legend()
ax.set_title("Model hysteresis loop")
plt.show()remanence Br = 0.570 T, coercivity Hc = 40 A/m, B at Hmax = 1.500 T
loop area = 239.7 J/m^3 per cycle
hysteresis loss at 50 Hz: 11.99 kW/m^3 = 1.57 W/kg
steepest slope at H = 40.0 A/m: mu_r(diff) = 11938
amplitude permeability at 200 A/m: B/(mu0 H) = 5502
The integrated area agrees with the rectangle estimate to 0.1 %. Note how many "permeabilities" one material has: about 12 000 on the steep part, 5500 as at , and almost 1 in saturation. Datasheets therefore quote the initial, the maximum and the amplitude permeability separately, and an inductor whose core saturates loses most of its inductance (Inductance of Common Geometries and Magnetic Energy).
Guided lab: display a ferrite's B-H loop
Hand calculation. A ferrite toroid with effective path length and area , turns. With in the primary, : gives , enough to drive a high-permeability ferrite towards saturation. The secondary voltage is ; an RC integrator (, , ) gives , so for these values.
Simulation. Adapt the model above: choose and from the ferrite's datasheet (typically around to , near ) and predict the loop.
What you would measure. Drive the primary from a function generator at through a sense resistor; channel X of the oscilloscope across the resistor (proportional to ), channel Y across the integrator capacitor (proportional to ), XY mode. You should see a loop that flattens at the ends; raise the amplitude to watch it saturate, lower it to see a thin ellipse (the Rayleigh region). Expect and within of the datasheet: the effective dimensions are approximations, the integrator droops, and ferrite properties change strongly with temperature. If the generator cannot supply enough current (its output limits it), add primary turns.
Hazards and safe setup. Signal-generator levels only (a few volts). Keep the oscilloscope grounds on the same side (both on the circuit's common), or one channel shorts the sense resistor through the ground leads (Probes).
Pitfalls
- Treating as a constant. Fine for small signals around a fixed point; wrong near saturation, with DC bias, or over temperature.
- Ignoring remanence. A core left magnetised (after a DC pulse or an interrupted transformer) can saturate on the next switch-on: transformer inrush current.
- Ferrite saturates early. About at room temperature and less when hot, against about for steel.
- Mixing up and for magnets. A magnet's useful field depends on both and on its shape (the demagnetising field); remanence alone does not say how strong a magnet is in use.
Practice
- A material has . What is , and what does give if it stays linear?
- With and in a steel, find .
- A ferrite core's loop area is at a given flux swing. What is the hysteresis loss at in a core of ?
Answer
- ; .
- .
- ; times = .
Test yourself
The general relation between B, H and M is…
The area of a B-H loop equals…
- the stored energy
- the energy lost per cycle per unit volume
- the permeability
- the remanence times the saturation
A material for a permanent magnet should have…
- low , low
- high , high
- high and a thin loop
Hysteresis loss at a fixed flux swing grows with frequency as…
Which core material saturates at the lowest flux density?
- silicon steel
- MnZn ferrite
- air
- iron powder