TExcelTAD
Home › Electrical Machines & Transformers › Hysteresis and Eddy-Current Losses: Steinmetz and Laminations

Hysteresis and Eddy-Current Losses: Steinmetz and Laminations

A distribution transformer is energised 8760 hours a year, and for most of those hours it carries a fraction of its rating. Its copper loss comes and goes with the load, but its core loss is there every second the supply is on. Over a transformer's life of several decades that loss can cost more than the transformer itself, which is why low-loss steels and amorphous cores exist and why efficiency regulations set limits on no-load loss. In a motor fed from an inverter at a few hundred hertz, core loss can become the largest loss of all. This lesson explains where core loss comes from, how the Steinmetz equation models it, and why every AC core is built from thin laminations.

Two mechanisms

Hysteresis loss. Each cycle round the B–H loop costs energy equal to the loop area per unit volume (Magnetic Materials, Permeability and Hysteresis): domain walls jump past pinning sites and the energy becomes heat. The loss per cycle depends on the peak flux density, so the power is proportional to frequency. Steinmetz fitted the dependence on the peak flux density with a power law:

Ph=kh f Bm n,n≈1.6 to 2.2 for silicon steelP_h = k_h\, f\, B_m^{\,n}, \qquad n \approx 1.6 \text{ to } 2.2 \text{ for silicon steel}

Eddy-current loss. A changing flux induces EMFs in the steel itself (Faraday's Law and Lenz's Law), and since steel conducts, currents circulate in loops around the flux and heat it. Splitting the core into thin sheets insulated from each other cuts the loops' area.

solid: one big eddy loop laminated: thin loops, thickness t flux into page, alternating same flux

For a sheet of thickness tt and resistivity ρ\rho, thin compared with the skin depth, a sinusoidal flux density of peak BmB_m gives a classical eddy loss per unit volume of

Pe=π2t2f2Bm26ρW/m3P_e = \frac{\pi^2 t^2 f^2 B_m^2}{6\rho}\quad \text{W/m}^3

The loss goes as the square of thickness and of frequency. Halving the thickness quarters it; doubling the frequency quadruples it. Silicon raises ρ\rho (pure iron about 0.1 μΩ⋅m0.1\ \mu\Omega \cdot \text{m}, 3 % silicon steel about 0.450.45 to 0.5 μΩ⋅m0.5\ \mu\Omega \cdot \text{m}) and helps twice, also lowering hysteresis loss. Measured losses are usually higher than the classical formula predicts: the extra part, called excess or anomalous loss, comes from the way domain walls move and is often modelled by a third term kexf1.5Bm1.5k_\text{ex} f^{1.5} B_m^{1.5}.

The total, in the form most often fitted to data, is

Pcore=khfBm n+kef2Bm2(W/kg)P_\text{core} = k_h f B_m^{\,n} + k_e f^2 B_m^2 \quad (\text{W/kg})

Worked example: why 0.35 mm sheets

Given: non-oriented silicon steel, ρ=0.48 μΩ⋅m\rho = 0.48\ \mu\Omega \cdot \text{m}, density 7650 kg/m37650\ \text{kg/m}^3, f=50 Hzf = 50\ \text{Hz}, Bm=1.5 TB_m = 1.5\ \text{T}.

Find: the classical eddy loss for 0.5 mm0.5\ \text{mm} and 0.35 mm0.35\ \text{mm} sheets, and the total core loss of a 12 kg12\ \text{kg} motor stator core with the loss coefficients fitted below.

Solve:

Pe(0.35 mm)=π2(0.35×10−3 m)2(50 Hz)2(1.5 T)26⋅0.48×10−6 Ω⋅m=2361 W/m3→23617650=0.309 W/kgPe(0.5 mm)=0.309 W/kg⋅(0.50.35)2=0.630 W/kg\begin{aligned} P_e(0.35\ \text{mm}) &= \frac{\pi^2 (0.35 \times 10^{-3}\ \text{m})^2 (50\ \text{Hz})^2 (1.5\ \text{T})^2}{6 \cdot 0.48 \times 10^{-6}\ \Omega \cdot \text{m}} = 2361\ \text{W/m}^3 \to \frac{2361}{7650} = 0.309\ \text{W/kg} \\ P_e(0.5\ \text{mm}) &= 0.309\ \text{W/kg} \cdot \left(\tfrac{0.5}{0.35}\right)^2 = 0.630\ \text{W/kg} \end{aligned}

The fitted steel below has 2.03 W/kg2.03\ \text{W/kg} at 50 Hz50\ \text{Hz}, 1.5 T1.5\ \text{T}. A punched and assembled core loses more than the Epstein-strip test sample (cutting stresses, burrs that short laminations, flux crowding in teeth), which designers cover with a building factor of about 1.31.3 to 22. With 1.51.5: P=12 kg⋅2.03 W/kg⋅1.5=37 WP = 12\ \text{kg} \cdot 2.03\ \text{W/kg} \cdot 1.5 = 37\ \text{W}.

Check: units: m2⋅Hz2⋅T2/(Ω⋅m)=V2/(Ω⋅m3)=W/m3\text{m}^2 \cdot \text{Hz}^2 \cdot \text{T}^2/(\Omega \cdot \text{m}) = \text{V}^2/(\Omega \cdot \text{m}^3) = \text{W/m}^3, since T⋅m2⋅Hz=V\text{T} \cdot \text{m}^2 \cdot \text{Hz} = \text{V}. The classical eddy part (0.31 W/kg0.31\ \text{W/kg}) is below the fitted eddy coefficient's 0.45 W/kg0.45\ \text{W/kg}; the difference is the excess loss.

In Python: separating the losses

The classic way to separate hysteresis from eddy loss is to test the same core at several frequencies and flux densities and fit the two-term model. The data below are synthetic test readings for one steel grade, in W/kg.

python · try it yourself
import numpy as np
from scipy.optimize import curve_fit
# loss of one steel grade measured at several frequencies and peak flux densities (W/kg; synthetic test data)
f = np.array([25, 50, 100, 25, 50, 100, 25, 50, 100, 200, 200, 200], float)
B = np.array([1.0, 1.0, 1.0, 1.3, 1.3, 1.3, 1.5, 1.5, 1.5, 1.0, 1.3, 1.5])
P = np.array([0.421, 0.916, 2.27, 0.668, 1.55, 3.7, 0.896, 1.99, 5.03, 6.04, 10.3, 13.4])

def model(X, kh, n, ke):
    f, B = X
    return kh * f * B**n + ke * f**2 * B**2

(kh, n, ke), _ = curve_fit(model, (f, B), P, p0=(0.01, 2, 1e-4))
print(f"kh = {kh:.4g} W/(kg Hz T^n), n = {n:.2f}, ke = {ke:.3g} W/(kg Hz^2 T^2)")
res = P - model((f, B), kh, n, ke)
print(f"worst fit error {np.max(np.abs(res / P)) * 100:.1f} %")
for ff, BB in ((50, 1.5), (400, 1.0), (400, 1.5)):
    ph, pe = kh * ff * BB**n, ke * ff**2 * BB**2
    print(f"{ff:3d} Hz, {BB:.1f} T: hysteresis {ph:6.2f} W/kg, eddy {pe:6.2f} W/kg, total {ph+pe:6.2f} W/kg")
kh = 0.01465 W/(kg Hz T^n), n = 1.91, ke = 7.91e-05 W/(kg Hz^2 T^2)
worst fit error 2.9 %
 50 Hz, 1.5 T: hysteresis   1.59 W/kg, eddy   0.45 W/kg, total   2.03 W/kg
400 Hz, 1.0 T: hysteresis   5.86 W/kg, eddy  12.66 W/kg, total  18.52 W/kg
400 Hz, 1.5 T: hysteresis  12.69 W/kg, eddy  28.49 W/kg, total  41.19 W/kg

At 50 Hz50\ \text{Hz} hysteresis dominates, three-quarters of the loss. At 400 Hz400\ \text{Hz}, the speed of a small high-speed spindle or aircraft generator, the eddy part takes over and the same core at 1.5 T1.5\ \text{T} would dissipate twenty times more per kilogram. High-frequency machines therefore use thinner sheets (0.10.1 to 0.2 mm0.2\ \text{mm}) and lower flux densities, and switch-mode transformers abandon steel for ferrite. Note that the fit is only valid over the range of the data: extrapolating a Steinmetz fit to frequencies or flux densities well outside the tested range is a common source of error.

Steel grades and what the datasheet says

Electrical-steel datasheets give the specific total loss in W/kg at a stated peak flux density and frequency, measured on Epstein strips or single sheets (IEC 60404-2 and IEC 60404-3 describe these tests). In the European naming (EN 10106 for non-oriented steel), a grade such as M270-35A means at most 2.70 W/kg2.70\ \text{W/kg} at 1.5 T1.5\ \text{T}, 50 Hz50\ \text{Hz}, in 0.35 mm0.35\ \text{mm} sheet. Grain-oriented grades are rated at 1.7 T1.7\ \text{T} and reach about 1 W/kg1\ \text{W/kg} or less; amorphous metal ribbons, used in some distribution transformers, reach a fraction of that at lower flux densities. (Grade names and standard numbers as of 2026; check the current editions.)

Separating losses at constant V/f

In a no-load test at constant V/fV/f the peak flux density stays fixed (from V=4.44fNABmV = 4.44 f N A B_m), so the core loss divided by frequency is a straight line:

Pcoref=khBm n+keBm2 f\frac{P_\text{core}}{f} = k_h B_m^{\,n} + k_e B_m^2\, f

The intercept is the hysteresis part per hertz, the slope the eddy part. This is how a lab separates the two from two or three no-load measurements on a real machine, and it is the experiment of the guided lab.

Guided lab: two-frequency loss separation on a toroid

Hand calculation. For the ferrite toroid of the previous lesson, pick a peak flux density well below saturation, say 0.1 T0.1\ \text{T}, and compute the drive voltages at 55, 1010 and 20 kHz20\ \text{kHz} with the EMF equation (each doubles with frequency: constant V/fV/f).

Simulation. Use the fitting program with your three readings: replace f, B and P and fit khk_h and kek_e with nn fixed at the datasheet value (fitting three parameters to three points has no check left).

What you would measure. Drive the winding through the 1 Ω1\ \Omega shunt as before and use the oscilloscope's math function to multiply winding voltage by current and average over whole cycles: that is the core loss plus a little copper loss (I2RI^2 R of the winding, which you subtract after measuring RR with a meter). Plot P/fP/f against ff. Expect losses of milliwatts to tens of milliwatts. The phase error between the two channels dominates the uncertainty: at a power factor near 0.10.1, a 1∘1^\circ skew changes the reading by about 17 %, so deskew the probes first (Probes) and treat the result as ±20 %\pm 20\ \%.

Hazards and safe setup. Signal-generator and audio-amplifier levels only, a few volts. No mains transformers or motors: their no-load loss tests are done by qualified staff with proper equipment, and this course treats them by calculation (Open-Circuit and Short-Circuit Tests).

Pitfalls

  • Extrapolating Steinmetz. The exponents change with flux density and frequency; refit for a new operating range.
  • Ignoring the building factor. A finished core loses noticeably more than the datasheet figure for the strip.
  • Forgetting harmonics. Inverter-fed machines see PWM ripple flux at kilohertz frequencies, which adds eddy loss far above what the fundamental predicts.
  • Burrs and damaged insulation. Shorted laminations behave like a thicker sheet, and the loss rises with the square of that thickness.

Practice

  1. A transformer core has a no-load loss of 120 W120\ \text{W} at 50 Hz50\ \text{Hz} and 160 W160\ \text{W} at 60 Hz60\ \text{Hz}, both at the same peak flux density. Find the hysteresis and eddy parts at 50 Hz50\ \text{Hz}.
  2. By what factor does the classical eddy loss change if the sheet goes from 0.50.5 to 0.27 mm0.27\ \text{mm} at the same ff and BmB_m?
  3. A transformer runs at 5 %5\ \% above rated voltage. Using the fitted n=1.91n = 1.91, estimate the rise in hysteresis and eddy loss.
Answer
  1. P/f=a+bfP/f = a + b f: 120/50=2.4=a+50b120/50 = 2.4 = a + 50b, 160/60=2.667=a+60b160/60 = 2.667 = a + 60b, so b=0.02667b = 0.02667, a=1.067a = 1.067. At 50 Hz50\ \text{Hz}: hysteresis af=53.3 Waf = 53.3\ \text{W}, eddy bf2=66.7 Wbf^2 = 66.7\ \text{W}.
  2. (0.27/0.5)2=0.29(0.27/0.5)^2 = 0.29: the eddy loss falls to 29 %.
  3. BmB_m rises 5 %: hysteresis ×1.051.91=1.098\times 1.05^{1.91} = 1.098 (about 10 %), eddy ×1.052=1.1025\times 1.05^2 = 1.1025 (about 10 %).

Test yourself

The classical eddy-current loss in a lamination is proportional to…

  1. tfBmt f B_m
  2. t2f2Bm2t^2 f^2 B_m^2
  3. fBm1.6f B_m^{1.6}
  4. t/ρt/\rho

Why is silicon added to electrical steel?

  1. to increase saturation flux density
  2. to raise resistivity and lower losses
  3. to make it non-magnetic
  4. to improve weldability

In a no-load test at constant V/fV/f, a plot of core loss divided by frequency against frequency gives…

  1. a parabola
  2. a straight line whose intercept is the hysteresis part per hertz
  3. a constant
  4. a straight line through the origin

The same core is operated at 400 Hz instead of 50 Hz at the same flux density. Which loss grows fastest?

  1. hysteresis
  2. eddy-current
  3. copper
  4. both equally